A) Preparation of kettle charge:Dissolve 36.00 parts of AEROSOL EF-800 in 270.00 parts of deionized water. Place in Kettle and heat to 80 oCB) Preparation of monomer charge:Add 120.00 parts of Styrene monomer in proper container.C) Preparation of CatalystDissolve 1.20 parts of Ammonium persulfate in 10.00 parts of deionized water.D) Addition of monomer charge to polymerization flask:When the contents of the polymerization kettle reaches 80oC, the nitrogen flow is reduced to a minimum and add monomer preparation as a shot to the reactor. Control reaction temperature between 85oC ~ 95oC with chilled water. After max exo thermic temperature holds for an hour. Cool to room temperature and discharge in proper container.